The Causes And Solutions Of SMT Processing Leakage And Less Tin

Dec 14, 2022

The causes of SMT processing leakage and low tin bad phenomena

1. Solder paste printing principle

After the squeegee squeezes the solder paste into the stencil hole, the solder paste touches the PCB surface and bonds to the PCB surface, and the solder paste stuck to the PCB surface overcomes the resistance of the stencil hole wall to transfer to the PCB surface when it is removed from the mould.

2. Observation, consideration, comparison

a. Printing although the pads around the substrate part of the area is covered by the stencil opening, but the stencil opening at the bottom of the solder paste is difficult to contact the PCB pads and surrounding substrate, not enough to overcome the resistance of the hole wall when demoulding (pads only a few solder paste)?

b. There is a 35 um deep circular pit between the pad and the solder resist, is the solder paste above the pit where the stencil opening is located not touching the bottom of the pit?

c. Why are the other pads connected to the line not easily missed?

3. Bare copper board printing verification

5 different brands of 4 powder solder paste can be in 0.1 thick, opening diameter 0.28 round hole stable under the tin (laser + electropolished stencil).

SMT processing leakage, less tin bad phenomenon solution

1. Find all the pads not connected to the outer line, the size of these pads from the original diameter of 0.27 round to 0.31 diameter round, reduce the area of the deep pits around the pads, so that the original in the deep pits on the open area becomes in the pad copper foil, so that the original in the deep pits on the open area and the stencil bottom gap is reduced. After the small batch verification OK, mass production using the original stencil, the original under the tin difficulties of the pad under the tin outstanding (increase the pad area, batch verification did not find even tin bad).

2. Reduce the thickness of the PCB solder resist, reduce the impact of the high solder resist layer on the line adjacent to the pad, the PCB solder resist thickness is less than 25um.

3. Choose a new type of PH stencil, the maximum elimination of printing gaps, PH stencil introduction.

ND2+N8+AOI+IN12C